1 coating method: high voltage electrostatic spraying friction electrostatic spraying
2 film thickness: 60 - 150um (according to the construction requirements of the adjustment)
3 surface treatment:
A. remove the surface of the oil, rust and other loose sediment, water, etc..
B. sand blasting or shot blasting treatment to Sa2.5 level, the anchor line depth of 40 - 100um
C. clean the pipe surface, the surface dust to near white level.
4 preheat, general control in the temperature range of 180220.
5 the powder coating is coated on the pipe surface by electrostatic spraying method, and the thickness is 60 - 150um.
6 will approximate the melting temperatures of hot melt adhesive in the winding construction in epoxy powder coating, the minimum thickness of 200um.
7 in the melting temperature of polyethylene surface (about 240 DEG C) during extrusion, winding in the middle layer construction, and the three layer of roller compaction, to prevent the bubble layer.
8 coating cooling.